In this project the pavement application of slag cement was used for durability, strength, ASR mitigation, and lighter color. Achieving close to 28-day flexural strength in 7 days 620 psi avg flexural strength. 28-day flexural strength of 700 – 750.
This is the first time slag cement was used in a Wyoming paving project. This is the first project Jacobs Eng said FAA has allowed slag cement in this Region.
This was a removal and replacement of the existing runway for the shared Wyoming National Guard and Cheyenne regional airport.
Application Type
|
|
% Slag Cement Replacement
|
35%
|
% Portland Cement
|
T I-II moderate alkali 0.60 -0.65, 680 lbs total cementitious 7.23 sk
|
% Portland Limestone Cement
|
|
% Other SCM (if applicable)
|
|
Aggregate
|
|
Water/cement ratio
|
0.38
|
7-day strengths
|
620 avg psi flexural strength
|
28-day strengths
|
700 – 750 psi flexural strength
|
Project Team
Owner: Cheyenne Regional Airport
General Contractor: Simon Contracting
Paving Contractor: S&S Builders
Engineer: Jacobs Engineering
Concrete: Croell Inc.
Slag Cement: Skyway Slag Cement